Can loss of oxidising species from the process liquor cause loss of passivity and rapid uniform attack of titanium heating tubes in acid service?

Nov 17, 2026

Leave a message

Titanium's corrosion resistance in acids is conditional, and the condition is the presence of an oxidising species. In aerated nitric acid, in dilute sulphuric acid containing dissolved oxygen or ferric ions, and in many process liquors with a positive redox potential, titanium builds and maintains a stable TiO₂ film and behaves as an inert material. Material selection charts quote impressive performance in these media, and designers reasonably conclude that titanium is suitable for the duty. The chart does not usually state the second half of the sentence: the same alloy in the same acid, with the oxidiser depleted, corrodes at rates that can be measured in millimetres per hour. This is the classic passivity-to-activity transition in titanium, and it is the single most common cause of catastrophic titanium failures that are subsequently reported as "unexplained". The oxidiser can be lost in ordinary, unremarkable ways: the plant switches from an aerated to a nitrogen-blanketed process; oxygen demand rises when organic material is introduced; ferric ions are reduced to ferrous by a change in feed; the vessel is closed and the headspace oxygen is consumed; a reducing agent is added for another process reason; or circulation stops and the residual oxidiser at the heater surface is consumed by the metal itself. In each case, the bulk analysis may still show "the same acid", and nobody samples for redox potential. Titanium gives no visual warning. There is no pitting, no crevice, no deposit: the surface simply begins to dissolve uniformly, stays bright for a while, and then roughens. Because the attack is uniform, the heater loses wall thickness evenly and the tube can fail across a whole section rather than at one spot.

The mechanism is the redox-potential dependence of titanium passivity. Titanium's oxide film requires an anodic oxidising agent to repair itself at the rate it is chemically dissolved by the acid. In reducing acid, the film dissolves and cannot regrow. The transition is sharp: once the potential drops below the critical value for the specific acid and temperature, the corrosion rate rises by several orders of magnitude, and the metal enters active dissolution with hydrogen evolution on its surface. Hydrogen uptake accompanies this, adding an embrittlement risk on top of the thickness loss. Temperature lowers the critical potential and raises the dissolution rate, so a heater, which is by definition the hottest surface in the vessel, is the first place to activate. The heater also has the highest local demand for oxidiser, since the reaction rate at the hot wall consumes dissolved oxygen faster than bulk mixing can replace it, which means that partial activation can begin at the heating surface while the bulk solution remains nominally in the safe range. Agitation and aeration are therefore not cosmetic process features for titanium service; they are part of the corrosion control system.

The signs are easy to miss or misinterpret: a change from bright metallic to a slightly grey, matte finish, an increase in dissolved titanium or hydrogen in the liquor, or a rise in the pick-up of corrosion products in the product stream. There is no pitting and no red rust, so the tube looks "fine, just a bit discoloured".

表格

Stage Surface Feature Electrochemical & Metallurgical State Risk Level Recommended Action
Marginal oxidiser level at the hot wall Bright surface, no visible change Local redox potential drops near the critical value at the hot zone Low Monitor redox potential at the heater, not only in the bulk
Film destabilisation at the heating surface Surface turns grey and matte, slight roughening Local activation begins, hydrogen evolution on the surface Medium Restore aeration or oxidiser dosing; reduce wall temperature
Active dissolution across the tube Uniform thinning, no pitting, bright etched texture Full passivity loss, corrosion rate rises sharply, hydrogen uptake High Take heater out of service immediately; measure wall loss
Section-wide failure Thinned wall collapses or splits over a large area Structural section below minimum for pressure and thermal load Critical Replace heater; install redox monitoring and interlock

Mitigation is chemical and operational rather than metallurgical, because switching to a higher titanium grade changes the threshold only slightly. Monitor redox potential or dissolved oxygen at the heater location, and interlock the heater so that it cannot run below the safe potential for the duty. Maintain aeration, sparging or oxidiser dosing as an explicit corrosion-control function in the operating procedure, not as an incidental process feature. Where the process must run under reducing conditions, titanium is the wrong material and should not be specified regardless of how good its performance was in the aerated pilot test. Keep the wall temperature as low as possible, since both the critical potential and the dissolution rate are temperature-dependent. Provide adequate mixing at the heater surface so that oxidiser is replenished rather than depleted at the metal.

Detection is chemical and dimensional. Dissolved titanium in the liquor is a direct indicator of active corrosion and is far more sensitive than waiting for a thickness change. Hydrogen content in the metal indicates the accompanying uptake. Ultrasonic thickness mapping taken on a fixed grid shows uniform loss that a visual check would miss. The most useful single instrument is an in-line redox or dissolved oxygen probe located downstream of the heater, where the depleted condition actually exists.

The common misconception is that a material compatibility chart stating "titanium is suitable for this acid" applies to all conditions under which that acid is handled. Titanium's suitability in acid is a function of oxidiser availability, and the chart describes only one point on that function. In summary, titanium depends on an oxidising environment to maintain its film, oxidiser depletion at the hot wall causes a sharp transition to active dissolution, and only redox monitoring plus deliberate oxidiser maintenance can prevent it.

info-717-483

Send Inquiry
Contact usif have any question

You can either contact us via phone, email or online form below. Our specialist will contact you back shortly.

Contact now!