Can zinc-induced liquid metal embrittlement damage 2205 duplex stainless steel heating tubes in hot-dip galvanising fume exhaust systems?

Nov 17, 2026

Leave a message

2205 duplex stainless steel is commonly used for heating tubes in exhaust gas reheating lines of hot-dip galvanising workshops, chosen for its high strength and chloride pitting resistance. Galvanising processes generate zinc vapour, fine zinc oxide particulates and condensed molten zinc aerosols that deposit on equipment surfaces. Most engineers only consider particulate abrasion and chloride corrosion in these exhaust streams, ignoring liquid metal embrittlement from molten zinc. When zinc deposits melt on the heater surface at temperatures above 419 °C, the molten zinc wets the stainless steel surface and penetrates grain boundaries under tensile stress. The dual-phase ferrite-austenite microstructure of 2205 shows uneven susceptibility: ferrite phases are more readily wetted by molten zinc, so crack initiation preferentially occurs within ferrite domains or along phase boundaries. The fracture appears brittle with little plastic deformation, and wall thickness remains nearly unchanged before rupture. This failure is extremely dangerous, as it can happen after months of stable operation without obvious surface corrosion.

The core mechanism is grain boundary wetting and cohesion reduction by molten zinc. Once molten zinc contacts stressed duplex steel, zinc atoms migrate along grain boundaries and phase interfaces. The metallic bonds between grains are weakened, and even moderate tensile stress can open intergranular cracks. Thermal cycling from intermittent heater operation creates alternating tensile and compressive stress, helping zinc continuously advance along crack paths. Zinc oxide deposits on the surface can also act as a reservoir: when the heater temperature spikes, oxide is reduced locally, producing fresh molten zinc to reinitiate embrittlement. Stress concentrations at welds, scratches and bend marks accelerate crack nucleation. Unlike conventional corrosion, this mechanism does not rely on metal dissolution; it is a physical-chemical degradation of grain boundary cohesion.

Early signs are limited to thin grey zinc deposits on the hottest zones. The metal surface looks intact, and only metallographic sectioning can reveal zinc penetration along grain boundaries.

表格

Stage Surface Feature Metallurgical State Risk Level Recommended Action
Zinc particulate deposition Thin grey zinc/oxide dust on hot surface Solid zinc accumulates, no wetting yet Low Install upstream filtration; reduce zinc aerosol loading
Melting and initial grain boundary wetting Glossy zinc droplets at hot spots Zinc melts, starts penetrating ferrite grain boundaries Medium Lower peak heater temperature; remove zinc deposits
Intergranular crack propagation Fine branching cracks visible after cleaning Zinc feeds crack tip, brittle crack growth High Remove heater for destructive metallographic inspection
Brittle fracture Flat brittle fracture surface, no ductile tearing Loss of grain boundary cohesion, sudden rupture Critical Replace component; use zinc-resistant alloy or barrier coating

Mitigation includes particulate filtration upstream of the heater to trap zinc aerosols, limiting peak operating temperature below zinc melting point where feasible, and regular mechanical cleaning to remove accumulated zinc deposits. Surface barrier coatings such as dense alumina can prevent direct contact between molten zinc and the steel substrate. Post-weld stress relief reduces tensile stress that drives crack opening.

A widespread misunderstanding treats zinc deposits as harmless dust. In summary, molten zinc wets ferrite grain boundaries of 2205 duplex steel, reduces grain boundary cohesion and causes brittle liquid metal embrittlement under tensile stress.

info-717-483

Send Inquiry
Contact usif have any question

You can either contact us via phone, email or online form below. Our specialist will contact you back shortly.